A glass furnace dust filter has to survive three stresses at the same time: flue gas that rarely falls below 350°C at the abatement inlet, batch carryover that condenses into sticky alkali-sulphate and borate films, and the 20–30 minute reversal of a regenerative melter that punches a dust spike through the vessel every time the firing side changes. Synthetic bags cannot live with that combination, and an electrostatic precipitator loses its nerve on sub-micron sodium fume. A rigid ceramic fibre candle does not. This article sets out what actually reaches the filter on a float, container or specialty melter, where conventional trains quietly lose the opex argument, how one ceramic vessel takes dust, acid gas, NOx and organic micro-pollutants together, and which numbers your enquiry has to carry before anyone can quote.

What actually arrives at the abatement inlet
Glass melting is one of the few industrial processes where the off-gas chemistry is set by the recipe rather than the fuel. Batch formulation, cullet ratio and melter type move the numbers more than burner adjustment does, which is why a filter quoted on gas volume and temperature alone is usually a filter that will be revisited during commissioning.
Temperature is dictated by the melter, not by the filter
On an end-fired or cross-fired regenerative furnace, most plants recover heat in a metallic recuperator or a fire-tube waste-heat boiler before the gas reaches abatement, and the filter therefore sees something in the 350–550°C band. Where there is no heat recovery, or where the plant wants the heat for batch and cullet preheating, the filter can sit much higher. Oxy-fuel melters are the opposite case: a much smaller gas volume, but a far more concentrated alkali and borate fume, because there is no nitrogen ballast to dilute what evaporates from the melt.
The particulate is fine, condensable and chemically aggressive
Two populations travel together. Coarse carryover comes from the batch blanket — soda ash, limestone, dolomite, feldspar and sand dragged out of the doghouse during charging. Fine fume forms inside the melter itself: sodium and potassium volatilise from the melt surface as hydroxides and chlorides, then re-condense as sulphates once the gas cools, producing a large fraction of particles well below one micron. On borosilicate and E-glass lines, B2O3 contributes low-melting borate films that behave less like dust and more like an adhesive. Fluoride raw materials release HF and SiF4; heavy-oil firing adds SO2, vanadium and nickel; selenium, cobalt and antimony appear depending on decolouriser and cullet mix.
Nothing about the duty is steady
A regenerative melter reverses roughly every 20–30 minutes. Each reversal purges the previously firing side, and during that window dust loading and temperature both step rather than ramp. Batch pushes and cullet charging add further transients. The melter itself will run for eight to fifteen years between rebuilds, so the abatement plant must never be the reason for a mid-campaign stop.
| Parameter | Range typically reported in glass enquiries | Why it matters to filter design |
|---|---|---|
| Filter inlet temperature | 350–550°C after heat recovery; higher on hot-filtration concepts | Sets consumption of cooling media and whether catalyst DeNOx is possible |
| Raw dust loading | 0.5–5 g/Nm³, higher during batch charging | Drives pulse frequency, hopper volume and whether a pre-separator is needed |
| Fine fraction | 60–90% of particle mass below 2.5 µm | Rules out purely inertial collection; demands true surface filtration |
| Condensible species | Na2SO4, K2SO4, borates, HF / SiF4 | Determines stickiness, chemical compatibility checks and alkali handling |
| NOx before abatement | Roughly 800–2,000 mg/Nm³ on air-fired melters | Sets whether a catalytic element plus ammonia injection is worth including |
| Moisture content | Combustion water plus batch moisture, usually kept below 20 vol% | Below the acid dew point the same dust becomes a cementitious deposit |
Treat those figures as orientation, not as a basis of design. Your own stack test, taken at two points in the reversal cycle and once during a batch push, is worth more than any table.
Why bags, ESPs and wet scrubbers struggle on glass melters
None of the three conventional routes is technically impossible. All three carry a recurring cost that does not appear in the comparison spreadsheet because it lands in maintenance budget rather than capital budget.
Fabric filters: the temperature ceiling
Standard aramid and PPS felts are rated for continuous service near 190–200°C. Treated glass-fibre fabric can push towards 260–280°C, which is still below where most melters leave you. The gap is closed either by water spray cooling — which adds vapour and moves the gas towards the acid dew point — or by blending dilution air, which inflates volume by tens of percent and forces a larger vessel and a bigger fan. Plants then discover that the bags still fail early, because alkali fume penetrates the needled felt, absorbs moisture during a cold start, and hardens into a layer that no amount of pulsing removes. The result is a rising baseline differential, a shortened campaign, and a bag change squeezed into a hot repair window.
Electrostatic precipitators: resistivity and fine fume
ESP collection efficiency depends on particle resistivity, and alkali sulphate fume sits squarely in the high-resistivity region where back corona begins: the dust layer breaks down electrically, re-entrainment rises, and efficiency falls just as the permit gets tighter. Because the fume is so fine, migration velocity is low, so the collection area has to be large. Operating near 400°C adds structural requirements for the casing and rapping gear, and SO3 or ammonia conditioning introduces another consumable. Even a well-run high-temperature ESP typically lands in the 20–50 mg/Nm³ band, which several permits no longer accept.
Wet scrubbing: swapping an air problem for a water problem
Scrubbers do remove HF and SO2 efficiently, and they will knock down some fine particulate. What they produce instead is a wastewater stream carrying fluorides, sulphates and trace selenium or antimony, plus sludge that frequently needs hazardous disposal. Saturated gas requires reheating before the stack, stacks plume visibly, and downstream ducting corrodes. For a plant without a discharge consent for that stream, this single point decides the whole project.
What changes when the filter media is rigid ceramic
A ceramic candle is a self-supporting element: it does not need a cage, it does not flex during pulsing, and it does not care about dust resistivity. Gas flows outside-in, so filtration happens at the outer surface rather than inside a felt thickness, and the deposit sits on a hard skin that a pulse can release in one piece. The detailed mechanism is set out on our filtration principle page, and the geometry and material options are listed under ceramic filter products.

Three consequences matter commercially. First, temperature stops being a problem to engineer around. Our elements run continuously at 600°C and tolerate short excursions to 1000°C, with the economic operating window sitting between 400°C and 1000°C. A glass furnace dust filter can therefore be placed where the gas is still hot, which means the heat downstream can go into a boiler or a batch preheater instead of into dilution air.
Second, pressure behaviour is predictable. A clean element measures 350 Pa at 1 m/min face velocity, and across our installed base the operating vessel differential settles between 900–1,500 Pa. Glass-industry duty typically sits in the narrower 900–1,300 Pa range, and that figure is what your induced-draught fan has to be specified against, including the transient during reversal.
Third, efficiency does not drift with resistivity. Collection efficiency holds at >99.99% because the barrier is the element wall, not a dust cake that forms and is then blown away. The standard geometry is φ150 × φ110 × 3,000 mm with a 20 mm wall, porosity >83%, manufactured to OD ±2 mm and length ±20 mm. Elements are supplied for a service life of more than 5 years and are backed by a 5-year written warranty.
Dust, acid gas, NOx and organics in one vessel
The strongest argument for ceramic candles on glass is not the temperature rating. It is that one vessel can carry four duties at once, because a ceramic candle is a support structure that happens to be a filter and can also happen to be a catalyst.
Acid gases: let the cake do the chemistry
Inject hydrated lime or sodium bicarbonate into the duct upstream of the vessel and the sorbent collects on the outer surface together with the dust. Every cubic metre of gas passing through that cake then contacts a large excess of alkaline surface, so HF, HCl and SO2 are neutralised on the way to the tube sheet. This is why the sorbent has in some situations to be part of the cleaning logic: pulse too aggressively and you throw away the reagent layer you are relying on for acid gas removal.
NOx: the window decides the layout
Where NOx is in scope — usually air-fired melters above roughly 1,000 mg/Nm³ untreated, or plants moving to oxy-fuel and losing their existing abatement margin — the practical answer is a catalytic version of the same element with ammonia injection upstream. Our catalytic ceramic fiber filter works across 170–300°C with an optimum between 220°C and 260°C, delivering about 90% DeNOx at 200°C and around 98% at 280°C. On most regenerative lines the gas leaving a waste-heat boiler lands naturally in that optimum band, which is why adding heat recovery is usually better engineering than trying to make the catalyst survive 450°C.
Running near the bottom of the catalytic window with sulphur present invites ammonium bisulfate condensation. Below 280°C we ask for SO2 to be held under 35 mg/m³ at the element — which the sorbent cake normally achieves — and we schedule a periodic 350°C × 12 h hold to decompose any deposit that does form.
Dioxins and organic micro-pollutants
A clean natural-gas float line has no meaningful dioxin load, and paying for catalytic destruction there is wasted money. That changes when the plant fires recovered oil, uses waste-derived fuel, or processes contaminated post-consumer cullet carrying organic residues. In those cases selective catalytic oxidation inside the same element removes dioxins up to 99.5% (TEQ), including the re-formation that happens as gas cools through the low-temperature synthesis range.
When dust control, sorbent injection, DeNOx and dioxin destruction are all configured together, the achievable stack figures are dust ≤1 mg/Nm³, SO2 ≤30 mg/Nm³ and NOx ≤50 mg/Nm³ (S.T.P., dry). Whether you need all four depends entirely on your permit; building the vessel so that modules can be added later is usually the cheaper decision.
Sizing and operating a glass furnace dust filter
Sizing mistakes on glass almost always come from reading the melting-end volume and forgetting what happens during reversal, so size against the transient rather than against the average.
- Face velocity. Design at or below 1.5 m/min. A standard element offers about 1.41 m² of external area, so at the 1.5 m/min catalog limit it handles about 2.12 m³/min; a 60,000 m³/h stream therefore needs at least about 473 elements before design margin. Split them into at least six compartments so one can be isolated while the melter stays online.
- Cleaning. Pulse at 0.35–0.55 MPa for 0.1–0.15 s, triggered on differential pressure rather than on a timer. On sticky borate-rich dust use the upper half of the pressure range; where the cake is doing acid-gas duty, let differential pressure rather than habit set the interval.
- Reversal transients. Give the fan real margin, size the hopper for the purge spike, and interlock compartment cleaning so that a pulse sequence cannot coincide with a reversal step.
- Mechanical tolerances. With OD ±2 mm and length ±20 mm, hold-down hardware has to be compliant. Use spring-loaded clamps and a gasket that absorbs variation rather than trying to torque against a hard stop.
- Chemical checks. Confirm free HF below 5 ppm at the element after any sorbent stage, confirm there is no phosphoric acid mist, and declare your Na2O and K2O loading. High alkali without an alkaline sorbent in the gas is a condition we need to design for rather than discover.
- Start-up. Bring the vessel above the acid dew point before introducing melter gas, and pre-coat with hydrated lime so the first sticky fume lands on a sacrificial layer rather than on clean ceramic.
Project snapshot: a flat glass producer in South China
A float line in South China came to us with a pulse-jet fabric baghouse that depended on dilution-air cooling to keep the media inside its rating. The operator was willing to share operating data but asked not to be named, so we describe the duty rather than the company.

Two costs were driving the review. Bags were being replaced roughly every fourteen months, and every change had to be fitted into a scheduled repair window because the baghouse had no meaningful bypass capacity. The dilution-air fan, meanwhile, was running continuously purely to protect the fabric, and every cubic metre of diluent was a cubic metre the plant paid to move and heat.
Conversion to ceramic candles removed both obligations. The vessel now runs between 420°C and 480°C without forced cooling, the operating differential settled inside the 900–1,300 Pa range that typifies glass-industry duty, and the plant’s own monitoring has held well below 5 mg/Nm³ since commissioning. Filter media is no longer a line item in the annual outage plan. The next phase under discussion is sorbent injection to bring HF within its own limit rather than relying on the particulate device alone.
If you are sizing something similar, our engineers will work from your gas analysis and, subject to the operator’s consent, arrange a reference discussion with the plant team.
Frequently asked questions
Can ceramic candles handle the gas temperature of an oxy-fuel melter?
Yes, and oxy-fuel is in some ways the easier case because the volume is small. Check instead the chemistry: oxy-fuel fume is concentrated alkali and borate, so we will want your Na2O, K2O and fluoride figures before confirming media formulation and whether sorbent injection is required ahead of the vessel.
Do we still need heat recovery upstream if we want DeNOx?
Usually yes, but for a different reason than you might expect. The catalytic window is 170–300°C with an optimum around 220–260°C, so a waste-heat boiler that brings gas into that band simultaneously pays for itself in steam and makes DeNOx possible in the same element.
What happens to acid gas removal while a compartment is being pulsed?
Removal efficiency dips briefly because part of the reactive cake has just been discharged. In practice the remaining cake and the continuous sorbent feed restore the layer within a pulse cycle, which is why we ask for differential-pressure triggered cleaning rather than aggressive timer-based sequences on abatement duty.
How do the elements cope with regenerator reversal every 25 minutes?
Well, provided the vessel is designed for the transient rather than the mean. Size the fan and hopper for the purge spike, interlock cleaning against the reversal sequence, and confirm the induced-draught machine can hold 900–1,300 Pa through the step rather than only at steady load.
What do you need from us to quote?
Gas volume at temperature, temperature profile including reversal excursions, dust loading and particle size distribution, SO2/HF/HCl, moisture, oxygen content, and your outlet limits. Add the batch recipe summary if you have it — alkali, boron and fluoride levels tell us more than any generic datasheet.
Send us your melter type, gas analysis and permit limits, and our engineers will return a first-pass vessel layout with element count, expected differential and whether DeNOx belongs in scope. Request a glass furnace filtration proposal.